Steel boats rust, and surface rust often goes much deeper than it looks. Get right down to good metal to find out what you're up against, then pick a repair to suit. For light surface rust, see removing rust, and once the steel's sound, coating a steel hull.

In this video, on the trawler, I go from light to heavy repairs: pad welding pits to build them back up (on the 4mm plate, 3.2mm rods at about 110 amps with a weave worked best), pad welding over a copper backing strap where the hole goes right through, welding a round patch in between two ribs, a doubler welded over a hole, and primer and filler over a pit above the fuel tank until I can empty the tank and fix it properly. Then I cut out the back deck and its ribs and weld in a new longitudinal, ribs and deck plates, using dogs and wedges to line the plates up. Damien's advice: don't be afraid to cut bad steel out and put new in. Keep new welds at least 100mm from other welds, as survey requires, and it's as strong as it ever was.

Plugging pinholes

In this video I plug small holes in Renko's deck. I drill them out with a 10mm bit, tap in a 12mm rod as an interference fit, weld round it and grind it flat. Spots that look like small pits can go right through once you chip them with a hammer, so you won't know the true extent until it's sandblasted.

Replacing a section of deck

The deck had a large rusted hole. In this video I pick where to cut back to good steel: a hole saw in each corner, cuts square to the coaming and parallel to the wheelhouse, and further out than I need where there's conduit underneath. I cut out the plate and the rusty base of the engine bay coaming, then make a template, tracing it from underneath. Later in the video I plasma cut the new plate from the template, bevel it, grind it bit by bit until it fits and tack it in. For the base of the coaming, I heat a length of flat bar on the stove and clamp it round the curve.

Forming a curved patch

Part of the sponson was too thin and pitted to pad weld, so in this video I cut it out and replace it. To get the new piece to the right curve, I run a weld down one side to hold it, and while it's still warm hammer it round the sponson. Then I break it off, cut the old bit out, and weld the new one in, closing the gap as I go.

Pad welding pits

In this video I pad weld low spots and pits on the hull and keel to build them back up, rather than filling them with a big lump of epoxy. I keep the heat low, 2.5mm rods at about 50 amps, so the metal doesn't sag. The trick is to match the rod to the depth: 3.2mm rods for a big depression on the keel, small 2mm ones for gaps, so there's less grinding afterwards. A deep, porous old weld gets a run up the middle and a Z-weave cap over the top. Then it's ground back ready for fairing compound.

Patching the hull and keel

Getting the hull ready for sandblasting. I TIG weld up the cuts left from taking off the old rubbing strip, and cut out a thin spot with a hole saw so a round patch can go in. Then I cut out and replace two thin sections of the 12mm keel, one that looks like it was caused by electrolysis, and make a new skeg. A new flat bar rubbing strip also goes on along the chine.

Testing the plate thickness

An ultrasonic thickness tester shows how much good steel is left. I clean up the corroded hull below the stern gland with a needle gun and wire wheel, explain how the tester works and how to zero it, then check a grid of points. The thinnest was 3.6mm, so that section stays.